Try this schedule. I’m
Home › Forums › Glassifieds › Stuff Wanted › problems with glass cracking when slumping › Try this schedule. I’m
May 29, 2012 at 3:24 am #12527
Participant
Try this schedule. I’m assuming you’re using COE90 glass. It looks like your second segment is too fast. New anneal temp is 900. Should work for 1/4″ to 3/8″ thick piece.
200/hr 900deg 30min
200/hr 1225deg 5min
9999 900deg 60min
100/hr 700deg 0min
200/hr 100deg 0min