I just throw them in with a large kiln-load, so it’s my “standard” fusing schedule (Sys 96) for two- to three-layer pieces:
Seg Rate Target Soak
1 150 1100 30
2 50 1250 60
3 250 1460 15
4 1500 950 90
5 100 700 00