Here’s a brief explanation of the schedule you posted:
ra 1 – 300 1175 .50 – initial heating and bubble squeeze
ra 2 – 300 1400 .10 – this is your process temp
ra 3 – full 960 .40 – rapid cooling and anneal hold
ra 4 – 100 800 .00 – anneal cooling
If you take a look at the firing schedules on this site (under “Tools” in the above menu) you will see that each segment of every schedule is explained. Simply reviewing several of those can teach you a lot about firing schedules.
Hope this helps
Paul