I have had screaming success with the following schedule;

425   1000   5

400   1100 10

full    1600    50

full     1500    20

full      950    2.00

300    300    0

Here is the fail part…I also did a Bullseye pot melt,(obviously a different anneal temperature),  FYI royal blue takes over everything!  Seriously.  Oh, and so does adventurine blue.  You would think I would have learned my lesson.  Oh well, I’ll just pot melt it again.

I believe I had about 3 pounds of glass, as my result was around 10″ or so.