Once you have established the temperature for the slump of that kind of project through observation, you can go back to the overnight firing.  I think you will find that you can often achieve your slump in this mould at 625 or 630C with a short soak rather than the 675C you did use. This will provide you with a less marked bottom surface.  Best wishes