I’ve successfully slumped
Home › Forums › Glass Fusing › General Fusing Discussion › Slumping Perrier Jouet bottle › I’ve successfully slumped
May 8, 2012 at 5:32 am #12520
Participant
I’ve successfully slumped two of them. The white does fade a bit, but it does ok. I actually do two firings on this one. The first one is in a bottle mold only to about 1350 for a 10 minute soak. The second firing is to 1400 on the shelf. This preserves the enamelling better with the lower temp and seems to keep the bubble out of the neck.