Here is the schedule I have for something that thick (in F):
Ramp Temp Hold (minutes)
68 1250 310
68 working varied
AFAP 930 1200
1.2 775 375
2.4 600 60
7.2 100 0
This is from a Spectrum Annealing chart I have. I cannot find a link to it online, or I would post it for you.