If I understand corrrectly, it’s the 19″ circles that are surrounded by the stainless rings .
I recently fired a very similar piece. I use System 96, so you’ll need to adjust your annealing temp, and potentially your top fusing temp. But my assumption is you are more interested in ramp rates, etc. Note that my 22″ blank was 3 layers, prefused. If you do not pre-fuse yours, you will need to include a bubble squeeze between 1100 and 1250. This is a 20 hour schedule:
Seg | Rate | Target | Soak |
1 | 150 | 1100 | 60 |
2 | 150 | 1325 | 15 |
3 | 1500 | 1000 | 60 |
4 | 50 | 950 | 240 |
5 | 50 | 800 | 00 |
6 | 100 | 700 | 00 |
I hope this is helpful — Dana