720C is right in the middle of the devitrification zone, so soaking for 30 minutes there is not a good idea. Try a long soak at ca. 677C or a quick one at 760C.  But the main thing is to have every thing very clean.  Contaminated surfaces, even if only a little, on bottles and float glass lead to devit very easily.